wood kiln

Wood drying is essential to ensure the quality and extend the life of wood and wood products. Appropriate measures must be taken to reduce the moisture content (moisture content) in the wood to a certain level.

Wood drying is a crucial step in ensuring and improving wood quality, reducing wood loss, and increasing its moisture content. Currently, artificial drying methods include conventional drying, high-temperature drying, dehumidification drying, solar drying, vacuum drying, high-frequency and microwave drying, and flue gas drying.

I. Stacking Requirements for Wood

Correct sticker placement, appropriate stack size, uniform stacking within the kiln, and good airflow conditions.

  1. Wood within the same drying kiln should be of the same species and have similar initial moisture content.

  2. The thickness variation of lumber within one kiln charge should not be excessive. When significant thickness differences exist, boards of the same thickness should be placed within the same layer to ensure each board is adequately pressed by stickers.

  3. Wood ends should be end-coated (e.g., with wax) to prevent end cracking.

  4. Correct Sticker Placement:

    • (1) Sticker spacing should be appropriate to minimize board deformation and ensure unobstructed airflow.

    • (2) Stickers should be placed perpendicular to the length of the stack. Stickers in adjacent layers should be vertically aligned and rest directly on the kiln truck’s support beams or cross-members to ensure normal ventilation and clear airflow channels within the stack.

    • (3) The distance from the sticker’s side to the stack end should be within one sticker width (≤30mm). Sticker length should match the stack width, and stickers should be of uniform width.

  5. Stacking within the Kiln:

    • Maintain a front-to-back spacing of approximately 10cm between stacks to prevent airflow blockage even if boards are misaligned.

    • Leave sufficient space (air channels) between the sides of the stacks and the back wall, and between stacks and the kiln door in the depth direction.

    • In the height direction, maintain a distance of 10-20cm between the top of the stack (or any weights on top) and the kiln ceiling.

  6. The length direction of the stack must be perpendicular to the airflow direction. Stacking lumber lengthwise parallel to the airflow is prohibited.

  7. Stacks should form a regular rectangular prism (cuboid). Stack sides should be straight and vertical. When lumber lengths vary, longer boards should be placed at the bottom and sides of the stack, while shorter boards should be placed in the middle and top to ensure stack stability.

  8. The airflow inlet (windward) side must be fully loaded with stacks; gaps are not allowed. If stack dimensions don’t match the kiln size or if the wood volume is insufficient, stacks can be staggered (cross-stacked) to prevent airflow short-circuiting and ensure drying quality.

  9. Stacks must be piled neatly and stably to prevent collapse during drying.

  10. Place weights (e.g., concrete blocks) directly over the stickers on the top layer to prevent warping of the upper layers.

  11. Operate kiln doors safely, moving them slowly and steadily according to procedure.

drying kiln

II. Preparation of Moisture Content Sample Boards (MC Measurement Point Selection)

Generally, wood moisture content refers to absolute moisture content. MC measurement is performed using several sets of probes located at different positions within the kiln. Probe positions should be selected on representative, visibly sound boards that are relatively wet. MC is measured by probes inserted into these boards. Additionally, select some non-online mobile sample boards placed at suitable locations within the kiln for testing and monitoring drying progress.

Alternatively, wood moisture content can be measured gravimetrically. For this, prepare MC sample boards. These boards should be selected from sound, straight-grained, knot-free, crack-free, visibly defect-free, representative, and relatively wet lumber.

lumber drying kiln

III. Schedule Selection

When drying wood, the appropriate drying schedule is primarily determined based on species, thickness, initial moisture content, and diameter (for logs). The schedule should be adjusted based on practical experience.

drying kiln for wood

IV. Implementation of the Wood Drying Process

  1. Preheating Treatment:

    • Purpose: Raise wood temperature uniformly throughout the stack, promote internal moisture redistribution, increase wood plasticity, prevent cracking and deformation, remove resins/extractives, sterilize, and improve dimensional stability.

    • During preheating, kiln temperature is typically slightly higher than the value specified for the equivalent MC stage in the schedule, or the relative humidity (RH) is set based on the wood’s initial MC and stress state. Preheating duration depends on species, thickness, and initial temperature. Generally calculated from when the kiln reaches setpoint conditions: Summer: 1–1.5 h/cm (thickness); Winter: 1.5–2 h/cm (thickness). The transition from preheating to the first drying schedule stage (equivalent MC) must take at least 2 hours.

    • (1) If Initial MC > Fiber Saturation Point (FSP) (no stress present): Use 100% RH (saturated air) to heat the wood rapidly.

    • (2) If Initial MC ≈ FSP: Use RH >96%. Allows slight surface moisture adsorption to reduce the MC gradient, restore deformability, and improve existing stress conditions.

    • (3) If Initial MC < FSP (residual deformation/stress present): Use RH in equilibrium with the wood’s current MC.

  2. Drying and Intermediate Conditioning:

    • After preheating, close steam valves, open vents, and gradually reduce dry-bulb/wet-bulb temperatures to those required for the first stage of the drying schedule. Schedule transitions must be gradual to prevent intense surface evaporation causing cracks if internal moisture diffusion ≠ surface evaporation rate. Operate inlet/outlet vents appropriately when adjusting kiln climate.

    • Never operate vents while injecting steam.

    • For refractory species or thick lumber, perform intermediate steam conditioning during drying to reduce moisture gradients and relieve stresses, preventing internal checks.

    • The timing, frequency, and duration of intermediate conditioning are determined case-by-case. Conditioning climate: Temperature slightly higher than or equal to the schedule temperature for the current MC stage; RH in equilibrium with the wood’s current MC. Conditioning duration: Approx. 1h steaming + 1-1.5h holding per cm thickness.

  3. Final Equalization and Conditioning:

    • (1) Equalization: Eliminate uneven MC distribution. Starts when the driest sample board is ~2% below target final MC and continues until the wettest boards reach the target MC. Climate: Temperature equal to the final drying stage temperature; RH in equilibrium with the MC of the driest wood.

    • (2) Conditioning: Reduce or eliminate residual stresses and through-thickness MC variation. Climate: Temperature equal to final drying stage; RH depends on species, generally in equilibrium with an MC 3% (softwoods) or 4% (hardwoods) above the final target MC. Duration: 2-6 hours per cm thickness.

  4. Cooling:

    • After drying completion, close heater and steam valves, open vents, and keep fans running. Cool wood to ~20°C above ambient outdoor temperature before unloading to prevent cracking.

drying kiln

V. Wood Drying Equalization and Conditioning (Seasoning)

  1. Conditioning After Kiln Drying:

    • After unloading from the kiln, wood must be stored in a dry shed for conditioning. This further evens out the moisture content within the wood and allows internal stresses to relax, effectively reducing residual stresses.

    • Conditioning duration depends on species, thickness, schedule intensity (mild/intense), use of intermediate/equalization treatments, and quality requirements. Therefore, it should not be rigidly fixed.

    • Duration and effectiveness should be determined based on monitoring dimensional stability of sample blanks and practical experience. Species with high density or abundant resin/oil canals generally require longer conditioning.

  2. Forced Moisture Equalization:

    • Forced moisture equalization rapidly balances MC and reduces internal stress.

    • If equalization during the final drying stage was inadequate (poor schedule control), forced moisture equalization (secondary drying treatment) must be performed on the blanks within the kiln. Stack the blanks according to drying requirements. Stacks must be square and stable, achieving “three straight sides and top surface with uniform pressure” . Stickers must be aligned vertically and weights applied on top.

    • Kiln dry-bulb temperature should be controlled at 40-50°C; higher temperatures risk cracking. Wet-bulb temperature is set based on the target final MC.

Get In Touch With Us